CMR 83/MMR 88

1. Examination of winding ropes—Under the regulations, winding ropes should be examined by the engineer or other competent person once in a week and every 30 days. In addition, a special examination of a portion of the rope cut off at the time of recapping is to be done.

It has been seen that the above examinations of winding-topes are not being done in a systematic manner and a note for guidance of persons concerned is given below.

The examination of the cut off portion of rope (including the portion in the cappel) at the time of recapping is particularly important as it would indicate the type of deterioration, if any, affecting the rope and the advance of that deterioration at the cappel end. The results of every such examination are to be recorded in a bound paged book, a specimen form for such record is enclosed.

It is also recommended that samples of rope after examination of recapping samples should be properly tagged and preserved for reference.

A NOTE ON EXAMINATION OF WINDING ROPES* *References : 1. A.E. McClelland. Pit Examination of Wire ropes.

2. N.C.B. Information Bulletin No. 55155.

3. The Ropeman's Handbook : N.C.B. Production Department.

I. Introduction—It is important to remember that anyone can make a routine examination and write in the Record Book 'in good order' after each examination, until the rope breaks. It takes a skilled person to make a useful examination and to make a note of how deterioration is advancing so that the senior officials can have the rope taken off before it breaks.

II. General considerations—(1) The first requisite for reliable rope examination and maintenance, is the careful selection of a competent person to be entrusted with this responsible work. The second requisite is that he should be given all available training.

(2) In examining a rope at the colliery the competent person should not merely look for broken wires. He should first endeavour to discover the type or types of deterioration affecting the rope as by the complete examination of recapping samples and should then note the symptoms of advance of such deterioration in other parts of the rope with a view to establishing the degree of deterioration reached.

(3) If the observations in such examinations are briefly but clearly recorded by the competent person in his own note book (apart from the entries in the Statutory Record Book) he will then have a case history for each rope readily available. These will be invaluable to him in advising his seniors regarding the date of discard of the rope concerned and will be very useful data for the maintenance and examination of later ropes working in the same position.

(4) Laboratory examination and testing of sample of rope by experts, where available, forms an extremely useful complementary service but the rope-man should be permitted to retain at the colliery sufficient length of each recapping sample for his own examination. Such laboratories can also help in giving instruction to the rope-man.

(5) Non-destructive methods of testing or inspection should not be regarded as possible alternatives to visual examination. Few of such methods are applicable to wire ropes and, even if these should prove entirely satisfactory in the future, they should be regarded as aid to normal inspection methods. Non-destructive methods of testing, and in fact all methods of testing, tend to measure the present condition of a rope without establishing the type of deterioration at work. Enlightened visual examination at colliery, or in the laboratory, establishes the type of deterioration and therefore enables a more accurate forecast to be made of the advance of deterioration.

III. Tools for rope examination—(1) Suitable calipers for measuring the rope diameter.

(2) A straight edge for measuring rope lay and micrometer gauge for measuring wire diameter and loss in wire diameter in opened samples of rope;

(3) A light hammer (a carpenter's cross pane pit hammer) with which to sound for loose outer wires and for corrosion product under those wires;

(4) A watchmaker's eyeglass, which can be held in the eye, to facilitate study of cracks, fractures and pits in wires;

(5) A tout bladed pocket knife with which to scrape off corrosion product and expose any pitting; the pocket knife might well have a slim and needle-pointed implement with which to explore the size and depth of scale-filled pits; and (6) A short sample length of each rope when new for ready comparison with the respective rope in service. Such a sample should be securely seized at each end, treated with lanoline to prevent corrosion and labelled for recognition purposes.

IV. Type of examination—Three types of examination are required by law for ropes used for raising or lowering persons. These are :

1. Weekly examination [Reg. 83(1) (b)/91 (1) (b) of the Coal/Metalliferous Mines Regulations].

2. Monthly examination [Reg. 83(1) (c)/91 (1) (c) of the Coal/Metalliferous Mines Regulations].

3. Examinations of recapping samples [Reg. 80(6)/88(6) Coal/Metalliferous Mines Regulations], Weekly examination—In weekly examination, the whole rope is examined roughly, by passing the rope at a speed not exceeding one metre per second, and only the more obvious faults can be sought (broken wired, loose wires, distortion or irregular lay in the ropes etc.).

When examining a preformed rope it must be remembered that broken outer wires are not easily found because their ends do not stick out of the rope. However, when the rope is passed slowly through a handful of clean cotton waste the broken ends usually pick up shreds of waste and thus draw attention to themselves. In addition, it is necessary to look carefully at the rope.

Monthly examination—This examination is to be made once at least in every 30 days, by passing the rope at a speed not exceeding 0.5 metres per second. For the purpose of this examination, the rope should be cleaned of any encrusted dirt and grease at all places particularly liable to deterioration and at other places, not more than 30 metres apart, throughout the length and any reduction in the circumference of the rope and the superficial condition of the wires as to wear, corrosion, brittleness and fracture of every such place in noted.

Special places to be examined are :

(i) the cappel end,

(ii) the rope over the headgear pulley with the cage at bank,

(iii) the rope leaving the drum with the cage at the bank,

(iv) the rope over the headgear pulley with the cage at pit bottom,

(v) the rope entering the drum with the cage at pit bottom, and (vi) any other places where deterioration is likely, such as :

(a) where the rope stands in the hooding in an upcast shaft,

(b) at the ends of the scroll where such a drum is used.

(vii) if the dead end of winding rope is anchored to the drum shaft, the piece of rope inside the drum must be examined.

It may be mentioned that cases of winding ropes breaking by fatigue inside the drum are known to be due to the rope inside the drum napping slightly as the drum rotates, thus causing fatigue where the rope is sharply and repeatedly bent at the rope hole. This trouble can be prevented by clamping the rope to a drum spoke or to straps fixed between two drum-spokes.

Better methods of fixing the dead end of the rope are by capping it and bolting the capping to the barrel or side of the drum, or to an internal or external rope reel.

Examination of recapping samples The regulations require that, except in Koepe system, before every recapping a length including the capping, of at least two metres shall be cut off the rope. Every piece of rope so cut off shall be opened and its internal condition examined. This is to be the most thorough examination, but as much of the procedure outlined below as possible, should also be carried out for the weekly and monthly examinations :

1. Diameter and lay—Measure the diameter across the crowns and not across the flats or valleys which would give too small a reading, See if it has lost a serious amount since the rope was new, say anything more than 5 percent (one twentieth) of the rope diameter when new. If it has, find out why, never accept a large, a sudden, or a local loss in diameter without searching for the cause.

If external wear is sufficiently heavy to explain the matter, the situation is not serious unless the wires are greatly reduced, and they should not be allowed to lose more than one-third of their thickness, If wear does not explain the loss in rope diameter, the trouble is probably internal and more serious. Internal corrosion may have eaten away the steel where the various wires touch one another, thus allowing the wires to draw closer together and shrink the rope.

An examination of the inside of the recapping sample will show if internal corrosion is increasing at the cappel end in which case it will be necessary to decide whether such corrosion might not be more advanced further up the rope. Tapping the outside of the rope with a light hammer should give a solid metallic sound and feeling. A dull sound will suggest that there is rust inside the rope. If the hammer bounces or chatters, the outer wires have become loose on the inner or core wires, perhaps due to internal corrosion. A stranded rope can be slightly reduced in diameter as a result of crushing of the fibre core, but this is not important.

Length of lay should also be measured from time to time, particularly at any point showing local distortion or reduction in diameter. A local increase in length of lay may indicate some serious internal fault such as a nest of broken inner wires.

2. Appearance of outside of rope—Note if there is any distortion of the rope, waviness, locked coil wire out of lock, looseness of outer wires, damage as distinct from deterioration etc.

Distortion, waviness and wires out of lock probably mean an accumulation of twist towards the cappel end, perhaps due to badly fitting pulley groove. Loose outer wires may be the result of untwisting in a rope or the result of a dangerous amount of wear or internal corrosion. Local damage may mean flapping and striking the detaching plate, a protruding rivet head or plate edge on the drum, something dropped down the shaft etc.

3. Condition of wires on outside—If there is external corrosion, consider whether the lubricant is suitable for the conditions and if it is renewed often enough. If wear is heavy, notice whether it is plastic which means heavy pressure against something. Other wear (abrasive) just means rubbing. Notice whether there is any chain pitting or other signs of surface embrittlement and if there are any broken-wires.

4. Condition of wires inside rope—The wires inside the rope can only be examined in the recapping samples cut from the rope unless a stranded rope in untwisted slightly while still in use. No attempt should be made without the consent and personal supervision of the engineer to untwist a rope while it is in use.

The examination of a sample rope should be commenced by measuring the diameter and lay, followed by an examination of the outside, and the sample should not be unlaid before this is finished. The inside should then be examined.

In the recapping sample of a stranded rope the condition of the fibre core should be noted whether it is lubricated or dry together with the condition of the wires touching the fibre (lubricated or dry, bright or corroded etc.). Then the condition inside the strands (lubricated or dry, bright or corroded, grooved or unworn etc.) should be examined. Broken or cracked wires and the position of the breaks (at the fibre core, where the strands touch one another etc.)

should, of course, be noted. Finally, decide whether the recapping sample is in any worse condition than the one cut off at the previous recapping.

With a locked coil rope. strip off and examine each layer separately. One layer can be removed without its wires becoming mixed with those of other, by seizing or clamping the sample about 3 inches from each end. Spring the ends of the outer layer apart as far back as the seizing and work another seizing under these ends to hold the remaining layers while the outer seizing and the outer layer of wires are removed.

Wires from the sample should be bent double, at least once in one direction and once in the opposite direction by hand, to see if they break at hidden fatigue cracks. Some outer wires from stranded ropes should be bent at worn crowns and some at other parts from inside the rope. If any wires snap regularly at worn crowns and nowhere else, it will probably be due to surface embittlement. If embrittlement has occurred, a number of hair cracks opening across the worn crown will be seen. A watchmaker’s magnifying glass with a magnification of 2 or 3 will be very useful for this work as it can be held in the eye, leaving the hands free.

When a wire is taken out of a strand of a Lang's Lay rope it will be wavy in shape and will show a large hump, followed by a small one, followed by a large one etc. The outside of a large hump lies on the outside of the rope where the external wear or worn crown will be found. The outside of the small hump lies against the fibre core and between the two will be found the nicks where the wires of one strand touch the wires of the next strand. The inside of the curves of humps represents the inside of the strand.

When studying fractures in wires, the type of the fracture and its position in the wire should be noted. This can be estimated from the brief explanation given earlier. From this it should be possible to decide the cause and find the remedy.

To find whether the steel in a galvanised or anti-corrosive rope is corroded or only the Zinc blackened, dip the wire into ordinary commercial concentrated hydrochloric acid (spirit of salt). The wire will fizz and bubble strongly until all the zinc has gone; this will take about half a minute. Clean the wire with waste, taking care not to get the acid on finger, or clothes.

Corrosion scale on the steel should be scraped off to find whether there are corrosion pits underneath. If there are, they should be prodded with a pin to find the depth and examined through the eyeglass at the same time.

It is important to remember that a wire is no stronger than its weakest part. A deep corrosion pit every 2 inches, with good wire between, is as serious as continuous pitting all along the wire. It is necessary to go about one 'rope lay' away from damage in a wire before getting clear of its effect on that wire. After such a distance the wire becomes locked in the rope by the surrounding wires and will take up its load again, even if broken.

Keeping Records—There is no point in making a careful and useful examination or rope if the results are not recorded. A written record of each rope should be kept for the use of ropeman and senior official, in addition to the entries made in the statutory Record Book. A separate book for each rope is best, giving the size, structure, maker's strength of the rope and whether it is galvanised or not, when it is put to work, and the usual rope life in that shaft. The note should include a record of all examinations, recapping. accidents etc. Examples of a suitable style for such notes are given below :

"Recapping sample 1/7/51.

Dia. I3732 in. Outside-well laid up, lubricant dry, zinc dark but steel O.K., light wear all round.

Inside fibre dry and nearest wires dry with dark zinc but steel O.K. Inside of strands well lubricated and bright. Only light nicking. No broken or cracked wires. Sample in sound order.

About the same as last sample." Six months later after the next recapping the following might be written :

"Recapping sample 1/1/52.

Dia. 11/16 in. Outside-well laid up, lubricant dry, zinc blackened and corrosion getting through to steel. Moderate wear all round.

Inside fibre and nearest wires dry with blackened zinc and small corrosion pits on steel.

Lubricant inside strands going blacky but wires still bright. Only light nicking. One outer wire cracked next to fibre, looks like corrosion-fatigue. Corrosion getting a hold. lubrication needs looking into." By doing this, the examination will begin to he of very real value.

Laboratory Test—If the recapping samples are sent to a testing station for examination and test, a visit to the station to see the tests carried out would be useful.

Tests carried out at Testing Stations are usually :

1. tension, 2. torsion, 3. reverse bending.

In tension testing the breaking strength of the wire is found in a testing machine and the sum of all the wire strengths gives the Aggregate Strength (not the Actual Breaking Strength) of the rope. The broken end of wire after this test will show a tension fracture.

In torsion testing the two ends of a length of wire are fixed in the two holders of a machine one holder being turned to twist the wire. This measures the 'ductility' (toughness and freedom from brittleness) of the wire and is an excellent way of finding small faults or fatigue cracks. A new ungalvanised wire will stand up to perhaps 36 twists over a length equal to 100 times the wire diameter, but the same wire with very small fatigue crack will probably break after two twists or less.

In reverse bend testing the wire is clamped in a vice fitted with specially rounded jaws and is bent backwards and forwards over these rounded jaws until it breaks. This also tests the ductility but over a very short length, and is of more use for new than worn wires.

When to remove a rope—Generally speaking a rope should be withdrawn from service when:

1. The factor of safety falls below 10 or such other limit fixed by Chief Inspector of Mines (i.e.

when the reserve of strength is no longer sufficient to ensure that the rope can repeatedly carry the shock loads, etc. with safety).

2. The loss of strength in the rope due to wear, corrosion or both is approaching 16% of the original strength.

3. The loss of strength in the rope due to fatigue, corrosion fatigue, surface embrittlement, or cracked and broken wires of any kind, is approaching 10% of the original strength.

4. The outer wires have lost about 15% of their depth as a result of any kind of deterioration.

5. The outer wires are becoming loose and displaced for any reason.

6. The rope has become kinked, distorted or damaged, and the damaged piece cannot be removed.

7. Examination of the rope leaves any doubt as to its safety for any reason whatsoever.

Form [See Regulation 80(6)/88(6) of Coal/Metalliferous Mines Regulations 1957/1961]

Record of Examination of Rope Serial No.

Colliery...............................................................................................................

Pit....................................................................................;............,.....................

Over or Under Rope............................................................................................

Date Cut Off.......................................................................................................

Date received.......................................................................................................

Type of rope........................................................................................................

Right or Left Hand Twist....................................................................................

Dia. Or Circ. or Width and Thickness..................................................................

Construction and size of wires............................................................................

External wear and corrosion................................................................................

Internal wear and corrosion.................................................................................

Lubrication and condition of core....................................I...................................

Broken wires.......................................................................................................

General Remarks................................................................................................

Signature..... Designation., Date.............

(Cir. 77/1963 and Tech. 1/1981)

Reproduced from the official DGMS circular compilations for public reference. The PDF is the authoritative text; DGMS may have amended or withdrawn older instructions since.

← Search all circulars